1. Introduction
Many scientific groups have been attracted by the properties of the wide band-gap III-V nitrides in the last years. The progress achieved in the control of the growth and doping of GaN, AlN and their alloys, Reference Morkoc, Strite, Gao, Lin, Sverdlov and Burns[1] and the successful application of these materials in the fabrication of optoelectronic devices, encourages increasing work on the characterization of the fundamental properties of these materials. The knowledge of these properties is important to determine the limits of their performance in device applications. Despite the successful fabrication of GaN/AlxGa1−xN heterostructures showing two-dimensional electronic properties Reference Redwing, Tischler, Flynn, Elhamri, Ahoujja, Newrock and Mitchel[2] and room-temperature stimulated emission, Reference Schmidt, Yang, Shan, Song, Salvador, Kim, Aktas, Botchkarev and Morkoc[3] the basic properties of AlxGa1−xN are, to a large extent, unknown. Reference Khan, Koide, Itoh, Sawaki and Akasaki[4] Reference Yoshida, Misawa and Gonda[5]
In this work, we study the Raman scattering spectra of AlxGa1−xN alloys grown by plasma-enhanced molecular beam epitaxy (MBE) and metalorganic chemical vapor phase deposition (MOCVD). The optical phonons have been studied as a function of the aluminum content x for the whole compositional range (0≤x≤1) for the MBE samples and for 0≤x≤0.5 for the samples grown by MOCVD.
Binary mixed crystals are classified into two main classes (one-mode and two-mode) according to the behavior of their optical phonons at the Γ point Reference Chang and Mitra[6]. In the one-mode class, the frequencies of the different optic modes vary continuosly and aproximately linearly when changing the concentration of the alloy. On the other hand, in the two-mode type behavior two sets of optic modes are observed, each set corresponding to one of the two pure crystals which compose the alloy. These “extra” modes may persist very close to the end compositions (x≈0 and x≈1). The modes occuring in the composition region where the materials are almost pure have been atributed to either a local or a gap mode arising from a residual concentration of the minority component.
An investigation of the Raman spectra of AlxGa1−xN films in the compositional range 0≤x ≤0.15 has been already performed. Reference Hayashi, Itoh, Sawaki and Akasaki[7] The authors analyzed the behavior of different phonon modes and could not find any evidence of a localized mode, finding a continous change of the energy of the modes as a function of aluminum concentration. Consequently, they concluded that AlxGa1−xN presents a one mode behavior. We have extended these studies to the whole compositional range of the alloy, analysing samples grown by two different methods (MBE and MOCVD). The experimental results are discussed in the light of recent theoretical calculations Reference Grille and Bechstedt[8] and conclusions about the quality of the samples are made.
2. Experiment
Substrates of (0001) sapphire were chosen to grow epitaxial AlxGa1−xN films by MBE and MOCVD to a layer thickness between 0.5 and 1 μm. The substrate temperature was maintained between 800 and 850°C during MBE growth. For the samples grown by MOCVD, the growth chamber was kept at a pressure of 100 mbar, and the substrate temperature was 950°C. Before the deposition of the GaN film, a thin buffer layer (≈50 nm) was grown at 550°C. For the MBE samples, however, no buffer layer was grown. The alloy composition was determined by elastic recoil detection analysis Reference Dollinger, Faustermann and Maier-Komor[9] (ERDA) and X-ray diffraction, with an absolute error smaller than 5%.
The Raman spectra were taken at room temperature in backscattering configuration from the (0001) surface of the wurtzite structure (z direction), and perpendicular to this surface (x direction). The Porto notation will be used to indicate the polarization configuration in which each spectrum was taken. The beam of an argon ion laser was used as exciting source (476.5, 488 and 515 nm). A microscope objective was employed to focus the laser on the sample surface to a spot size of about 2 μm, with a power density of about 105 W/cm2. The Raman signal was analyzed with a triple spectrograph and detected with a cooled CCD camera. The lattice mismatch between film and substrate induces stress in the samples, which reflects in a shift of the phonon modes in the Raman spectra. This stress has been investigated by means of X-ray diffraction, and the corresponding Raman shift has been estimated to reach a maximum value of 3 cm−1. Reference Rieger, Metzger, Angerer, Dimitrov, Ambacher and Stutzmann[10]
3. Discussion
To study the Raman selection rules, which allow the assignment of the phonon modes, we have plotted in Figure 1 the Raman spectra of an AlxGa1−xN sample with 50% aluminum, measured in four different polarization configurations. This sample was grown by MBE under the same conditions as the other samples measured in this work. The only difference is that its thickness is somewhat greater (3μm), to facilitate the measurement in the
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170811042620675-0788:S1092578300001691:S1092578300001691_eqn1.gif?pub-status=live)
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170811042620675-0788:S1092578300001691:S1092578300001691_eqn2.gif?pub-status=live)
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170811042620675-0788:S1092578300001691:S1092578300001691_eqn3.gif?pub-status=live)
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170811042620675-0788:S1092578300001691:S1092578300001691_eqn4.gif?pub-status=live)
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170811042620675-0788:S1092578300001691:S1092578300001691_eqn5.gif?pub-status=live)
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170811042620675-0788:S1092578300001691:S1092578300001691_fig1g.gif?pub-status=live)
Figure 1. Room temperature Raman spectra of an AlxGa1−xN sample with a thickness of 3μm and an aluminum content of 50%. The polarization configuration used is indicated on each spectrum.
Figure 2 shows some of the Raman spectra obtained in the
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170811042620675-0788:S1092578300001691:S1092578300001691_eqn6.gif?pub-status=live)
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170811042620675-0788:S1092578300001691:S1092578300001691_fig2ag.gif?pub-status=live)
Figure 2a. Room temperature Raman spectra obtained for different AlxGa1−xN compositions. Spectral range showing (a) A1(TO) (green triangles) and E2 (red dots and black arrows) phonon modes. The dashed line indicates the position of the modes related to the sapphire substrate.
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170811042620675-0788:S1092578300001691:S1092578300001691_fig2bg.gif?pub-status=live)
Figure 2b. Room temperature Raman spectra obtained for different AlxGa1−xN compositions. Spectral range showing A1(LO) phonon mode (blue triangles). The dashed line indicates the position of the modes related to the sapphire substrate.
As the aluminum content of the alloy is increased, the phonon modes shift to higher energy, but the E2 line changes its energy much more slowly than the A1(LO) and A1(TO) lines. An interesting feature arises for an alloy composition of 36% aluminum, where a new mode is observed as a broad peak centered at 629 cm−1. The intensity of this line increases with increasing aluminum content, and it shifts slowly to higher energy towards the position of the E2 line of AlN. The line is indicated by arrows in the different spectra of Figure 2a. At the same time, the intensity of the E2(GaN) mode decreases, and for an aluminum content greater than 89% the peak cannot be detected anymore. This behavior indicates the existence of one E2 mode characteristic of GaN and one characteristic of AlN for an intermediate alloy composition (two-mode behavior).
A better insight into the behavior of the different phonon modes can be obtained from Figure 3, which shows the position of the phonon modes as a function of aluminum content. The A1(LO) (blue triangles) shows a one-mode behavior, although its dependence on aluminum content is not linear. In the region of 600 cm−1, the two mode behavior of the E2 mode (red dots) can be clearly seen. As can be seen in Figure 3, both modes (E2(GaN) and E2(AlN)) have been simultaneously measured for an alloy composition ranging from 35% to 66% aluminum. The behavior of the A1(TO) phonon mode (green triangles) is unfortunately not so clear. We have looked for an AlN local mode by measuring in the
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170811042620675-0788:S1092578300001691:S1092578300001691_eqn6.gif?pub-status=live)
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170811042620675-0788:S1092578300001691:S1092578300001691_fig3g.gif?pub-status=live)
Figure 3. Dependence of the frequencies of the A1(TO) (green triangles), E2 (red dots) and A1(LO) (blue triangles) phonon modes on alloy composition.
In Figure 4 we compare the Raman spectra from the MBE (black line) and MOCVD (blue line) samples for two typical samples with 19% aluminum content. The width of the E2 phonon peaks of both samples are comparable (7 vs. 8.5 cm−1, see also Figure 5). However, a striking difference between both spectra is the presence of the A1(TO) phonon mode in the MBE sample, which is absent for the MOCVD sample. This line should be forbidden in backscattering from the c axis of the wurtzite structure, as we already mentioned in the discussion of Figure 2. It must also be pointed out that the position of the E2 phonon mode is slightly different for both samples (the peak of the MBE sample shifts 2 cm−1 to higher energy), although their aluminum content is almost the same. The difference in peak position and presumably also the failure of the selection rules in the
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170811042620675-0788:S1092578300001691:S1092578300001691_eqn6.gif?pub-status=live)
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170811042620675-0788:S1092578300001691:S1092578300001691_fig4g.gif?pub-status=live)
Figure 4. Room temperature Raman spectra of two AlxGa1−xN samples grown by MBE (black) and MOCVD (blue) with an aluminum content of 19%. The spectrum of a sample with only a GaN buffer layer grown by MOCVD (red line) has been included for comparison with the spectrum plotted in blue. The dashed line indicates the position of the sapphire Eg mode. The arrows indicate the A1(LO) phonon mode arising from the GaN buffer layer.
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary-alt:20170811045333-05930-mediumThumb-S1092578300001691_fig5g.jpg?pub-status=live)
Figure 5. Dependence of the linewidths of the E2(GaN) (full dots) and E2(AlN) (empty dots) phonon modes on aluminum content for the MBE (red) and MOCVD (green) samples. The lines are drawn as guides to the eyes. The inset shows the relative intensities of the E2(GaN) and E2(AlN) phonon modes as a function of aluminum content
The peak centered at 730 cm−1 (arrows), which appears in the spectrum of the MOCVD sample, arises from the GaN buffer layer (A1(LO) phonon mode). This has been determined by measuring a sample with only the buffer layer, whose spectrum is shown at the bottom of Figure 4 (red line) for comparison with the spectrum of the MOCVD sample (blue line).
The widths of the E2 phonon modes are compared in Figure 5 for both types of samples, where the full width at half maximum (FWHM) is shown as a function of alloy composition. The linewidth of the GaN E2 mode quickly increases with aluminum content, while the AlN E2 mode becomes narrower. The decrease of the linewidth of the E2(AlN) mode is observed in the MBE as well as in the MOCVD samples, and it cannot be attributed to a change in the crystalline quality of the samples. This behavior seems therefore characteristic of the mode itself. In the inset of Figure 5 we have plotted the relative intensities of the Raman signals of the E2(GaN) and E2(ALN) phonon modes as a function of aluminum content. It can be seen that the strength of the E2(AlN) line increases with respect to the E2(GaN) as the aluminum content is increased from 30% to 70%, as expected in a two-mode type semiconductor. Reference Barker and Sievers[16] The maximum observed for x=0.8 in the linewidth of the E2(AlN) phonon mode correlates with the crystalline structure of the alloy as studied by X-ray diffraction, and is attributed to stress and a higher structural disorder. The linewidth of the E2(GaN) phonon mode is comparable for the MOCVD and MBE samples up to an aluminum concentration of 30%. For higher concentrations the phonon line of the MOCVD samples becomes much broader, indicating a deterioration of their crystalline quality.
4. Conclusions
We have characterized the behavior of the optical phonons in AlxGa1−xN films by means of micro-Raman spectroscopy. Both one and two-mode behavior are simultaneously observed in this III-V alloy system for different phonon modes. While the A1 phonon modes seem to show a one-mode behavior, the E2 phonon modes exhibit a two-mode type behavior. From the extrapolation of the data shown in Figure 2, the frequency of the Al local mode in GaN is estimated to be 616 cm−1, while the Ga gap mode in AlN would vibrate at 605 cm−1. The Raman spectra of samples grown by MBE and MOCVD have been compared, discussing the selection rules for the phonon modes, and conclusions about the quality of the layers have been drawn.
Acknowledgments
One of the authors (A.C.) would like to thank the Ministry of Education of Spain for financial support and the Walter Schottky Institut for its hospitality.