Introduction
While III-nitride epitaxy offers great potential for optoelectronic, high temperature and high power devices, the common use of sapphire has many disadvantages. The use of single crystal III-nitride substrates should allow improved epitaxial growth, improved thermal and chemical compatibility, as well as improved thermal conductivity.
We have succeeded in growing single crystals of AlN exceeding 1 cm in length and 0.5 cm in diameter using the technique of sublimation and recondensation [Reference Slack and McNelly1]. Substrates of AlN have been cut from these single crystals boules with either the (11
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170731073217724-0817:S1092578300002817:S1092578300002817_eqn02.gif?pub-status=live)
Growth Procedures
All growths were carried out in an rf-heated, hot-wall, horizontal reactor [Reference Lu, Bhat, Ponce, Dupuis, Nakamura and Edmond2]. The growth temperature was 1100 °C, while the growth pressure was 100 torr. Trimethylaluminum (TMA), trimethylgallium (TMG) and ammonia (NH3) were used as the source materials, and the carrier gas was hydrogen. An AlN substrate and a c-plane sapphire substrate were placed side by side to compare epitaxial quality and calibrate the growth rate. After a chemical clean and prior to the epitaxial growth, the substrates were thermally treated at 1100 °C under 2 slm of hydrogen flow for 5 min and under a mixed stream of 1slm ammonia and 2 slm hydrogen for 10 min. After this treatment, the flow rates of H2 and NH3 were adjusted to 3 slm and 2 slm respectively, and then TMA (for AlN growth) or a combination of TMA and TMG (for alloy growth) was switched into reactor. In all cases, the flow rate of TMA was 30 sccm.
Under these conditions, the AlN growth rate was about 0.5 μm/hour (for the sapphire substrate) as determined by FTIR measurements. Typical growth times were about 1.5 hours. The 50% alloy discussed below was achieved with 3sccm and 30sccm flow rates of TMG and TMA, respectively. Doping was accomplished by using 11.1 ppm silane in a hydrogen carrier gas.
Characterization and Analysis
In Fig. 1, an AFM image of an AlN substrate is shown prior to epitaxial growth. This particular substrate was cut so as to expose the (11
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170731073217724-0817:S1092578300002817:S1092578300002817_eqn02.gif?pub-status=live)
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary-alt:20170731083524-37516-mediumThumb-S1092578300002817_fig1g.jpg?pub-status=live)
Fig. 1: An AFM image of the bare AlN substrate prior to growth.
In Fig. 2, an AFM image of a 0.7-μm-thick AlN epitaxial layer, grown on a slightly vicinal AlN substrate, is shown. Atomic steps seem to have organized into semi-regular arrays during growth giving rise to a grating effect across the surface. The height of the step bunches is approximately 4 nm. The density of defects across the surface, observed with AFM, increased by approximately 1 order of magnitude from the clean substrate. This increase includes the appearance of short line-like defects that were not observed on the original substrate. The origin of these defects is still being investigated.
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary-alt:20170731083524-78563-mediumThumb-S1092578300002817_fig2g.jpg?pub-status=live)
Fig. 2: An AFM image of a 0.7-μm-thick epitaxial AlN layer grown on the a-face of an AlN substrate.
We have also performed AFM characterization of the surface of a 1-μm-thick epitaxial film of Al.5Ga.5N. This film showed a much rougher surface morphology even though the epitaxial quality as determined by x-ray diffraction and ion channeling was very good as discussed below. The surface was found to have many mounds on the surface with approximately 30° facet angles. Of course, it should also be noted that the growth process has not yet been optimized for growth of AlxGa1−xN alloy layers.
Rutherford backscattering/ion channeling measurements were used to determine the crystal quality of the original substrate, the epitaxial AlN layer and the epitaxial Al.5Ga.5N layer. The results from the later two layers are shown in Figs. 3 and 4. These measurements were performed at the SUNY-Albany Dynamatron accelerator with 2 MeV He4 ions. The minimum yield was measured along the [10
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170731073217724-0817:S1092578300002817:S1092578300002817_eqn01.gif?pub-status=live)
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170731073217724-0817:S1092578300002817:S1092578300002817_eqn02.gif?pub-status=live)
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary-alt:20170731083524-98937-mediumThumb-S1092578300002817_fig3g.jpg?pub-status=live)
Fig. 3: RBS spectra measured for a random direction and along the [10
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170731073217724-0817:S1092578300002817:S1092578300002817_eqn01.gif?pub-status=live)
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary-alt:20170731083524-29473-mediumThumb-S1092578300002817_fig4g.jpg?pub-status=live)
Fig. 4: RBS spectra measured for a random direction and along the [10
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170731073217724-0817:S1092578300002817:S1092578300002817_eqn01.gif?pub-status=live)
Note also in Fig. 3 that some Ga contamination is seen in the epitaxial film. The Ga concentration is approximately 1% and helps to serve as a marker for the epitaxial AlN film. The ion channeling minimum yield on the AlN/sapphire layer grown under identical conditions was 40%.
The insets in Figs. 3 and 4 show the onset of the Al and the Ga peaks, respectively. In Fig. 3, the surface peak is due to the scattering of the He ions by Al ions on the surface prior to the He ions starting to channel in the crystal. In Fig. 4, it is interesting to note that the Ga surface peak is nearly missing in spite of the fact that the alloy was grown under constant TMA and TMG flux. This suggests that the surface layer is depleted of Ga and suggests that some surface reconstruction may have occurred which preferentially put Al on the surface. Another possibility is that the epitaxial layer preferentially lost Ga during the cool down phase after growth.
Double crystal, x-ray diffraction (Bede diffractometer, Cu K α ) radiation was also used to characterize the quality of the epitaxial layers. A GaSb (004) reflection was used to monochromatize the x-rays and the (11
![](https://static.cambridge.org/binary/version/id/urn:cambridge.org:id:binary:20170731073217724-0817:S1092578300002817:S1092578300002817_eqn02.gif?pub-status=live)
The Al.5Ga.5N alloy was doped with Si as described above using a silane/hydrogen flow rate of 3 sccm. The 1-μm-thick film exhibited a resistivity of approximately 20 Ω-cm. Hall measurements were made using In dots that allowed good Ohmic contacts to be made to the epitaxial layer. The concentration of carriers was approximately 1017 cm−3 with a mobility of ∼10 cm2/V-s. Generally groups have found that doping of AlxGa1−xN alloys is difficult at high Al fraction [Reference Zhang, Kung, Saxler, Walker, Wang and Razeghi5,Reference Redwing, Flynn, Tischler, Mitchel, Saxler, Ponce, Dupuis, Nakamura, Bremser and Edmond6] probably due to the inferior material quality. Our results here are in good agreement with Bemser et al. [Reference Bremser, Perry, Nam, Griffis, Losing, Ricks and Davis7] for high concentration Al alloys grown on 6H-SiC(0001) substrates.
Conclusion
We have demonstrated that a-face AlN substrates can be prepared for excellent homoepitaxial growth of AlN. In addition, we have demonstrated high quality alloy growth of Al.5Ga.5N on these substrates that showed excellent electrical conductivity even though the growth conditions were not optimized. The AlN substrates offer an excellent opportunity to achieve high quality epitaxial growth of AlGaN alloys on a high thermal conductivity, electrically insulating substrate with minimal thermal expansion mismatch.
Acknowledgements
The contributions of Jonathan Ward in substrate preparation are hereby gratefully acknowledged. This work was partially supported by the Ballistic Missile Defense Organization (BMDO) and ONR. The support and advice of Dr. C.E.C. Wood at ONR was greatly appreciated. In addition, Crystal IS received support from BMDO and was managed by the Materials Directorate of the Air Force Research Laboratory, USAF, Wright-Patterson AFB.